search  current discussion  categories  glazes - misc 

glaze of week may 26 2000

updated wed 31 may 00

 

hal mc whinnie on thu 25 may 00


HAL'S PALE APPLE GREEN MATT
CONE 7-10
REDUCTION

zinc oxide 7
custer spar 40
cornwall stone 20
whiting 20
epk 20
bento0nite 2
yellow ochre 6
light rutile6

A GOOD MATT GLAZE WITHOUT BARIUM

can be fired oxidation or reduction

Kris Bliss on fri 26 may 00


> HAL'S PALE APPLE GREEN MATT

> light rutile6
>
> Quick question.. what is light rutile ? can i use ceramic rutile ?
Thanks in advance, i plan to test this asap and will let you all (ya'll)
know how it works for me..
kris in Ak.
sunrise today 4:30 am sunset 11:10 pm
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.