search  current discussion  categories  glazes - cone 4-7 

temoku-like at cone 6, was glaze recipes for all & a note to ron roy

updated sat 10 jun 00

 

Michelle Lowe on fri 9 jun 00


Hi Andie,

I did a lot of cone 6 (ish) testing for a few years, I didn't really find a
glaze just like a beautiful temoku, but I did get a couple really nice
"iron saturate" glazes that would go black, to brown, to brick red
depending on clay/firing speed/cooling speed etc.

Here they are-

Super Deluxe Cone 5-8

Flint 24
EPK 4
Kona F4 16
Talc 11.2
Gerstley 25.6
Red Iron Ox 21.1

black/brown breaking to cobalt blue where thin
brick red with two coats dripping khaki


And-

Iron Brown (goes red when refired at 08-04) cone 4-7
>
>Silica 25
>Custer Spar 17
>Talc 12
>EPK 4
>Gerstley Bor. 36
>
>RIO 25 (yeah I know, it's a lot!)
>
>Very nice mottled brown/green sometimes almost black

Michelle Lowe, potter in the Phoenix desert \|/ |
mishlowe@amug.org -O- | |
mishlowe@aztec.asu.edu /|\ | | |
|_|_|
____ |
http://www.amug.org/~mishlowe -\ /-----|-----
( )
<__>