hal mc whinnie on tue 20 jun 00


i will continue with my cone 5 glazes. these glaze formulas are also being
circulated on my own address lists which number about 2,000. I regret some
of the overlaps and some do get two copies, one set on my lists and the
other on clayart.

hal's majolica one

cone 5

frit 25 55
china clay40
FLINT5
tin oxide8
RUTILE 3

not based on 100 percent

hal's majolica two

cone 5

frit 25 36
frit 399 24
custer spar 31
china clay 13
flint 18
tin oxide 5
copper carb 3

not based on 100 percent