Receipe

Custer feldspar 51,0 (used the one I had available, =
feldshammer)
Whiting 18,6
Kaolin 10,8
Zinc.ox. 8,7
Silica 5,9
Bentonite 4,9

ADD
cold. carb. 1,0%

Glaze is consistent and has shiny surface with a typical colbalt blue =
color.
Not exciting but stable. Gives a very dark marine blue where thickest.
Intereacted fine with a transparent, white and a darker blue I
tested it over.