Receipe=20

Potash feldspar 40
Ball clay (Hvar) 15 used the one I had avail.=20
Silica 20
Whiting 15
Zinc. ox. 15

ADD
titanium ox. 10%
Colb. ox. 0,75%
Copper ox. bl. 1,0%

Strong blue to yellow brown, shiny.
Results were consistent with a stong marine to turquoise blue where =
thicker, brownish yellow edges where thin.
Also had blue spots in thinner areas. Had some "Blue Hare" effect, with =
a blue rain within a brownish ground.
A varying glaze depending on thickness.

Could be a keeper because I like the variance of nuances and the =
materials are commonly found.