search  current discussion  categories  glazes - misc 

need oatmeal glaze pls

updated thu 10 aug 00

 

CSLPZZN@AOL.COM on mon 24 jul 00


I'm looking for an Albany glaze called Oatmeal Matte. It's fired to ^6 Ox.
I couldn't find it in the archives and I believe that a friend sent it to me
from another web sight. We've searched everywhere with no luck.

It's a beautiful, warm, toastie. semi gloss cream. When I ran out of Albany
I tried Alberta....yeesh....that pot went off the cliff. Now I have another
stash of Albany...I had since thrown out the recipe thinking I'd never gets
my hands on Albany again.

Can anyone help?
Thank you
Carolyn

Diane G. Echlin on tue 25 jul 00


I believe if you search the archives for "Pike's Oatmeal" you will find what you
are looking for.

CSLPZZN@AOL.COM wrote:

> I'm looking for an Albany glaze called Oatmeal Matte. It's fired to ^6 Ox.
> I couldn't find it in the archives and I believe that a friend sent it to me
> from another web sight. We've searched everywhere with no luck.
>
> It's a beautiful, warm, toastie. semi gloss cream. When I ran out of Albany
> I tried Alberta....yeesh....that pot went off the cliff. Now I have another
> stash of Albany...I had since thrown out the recipe thinking I'd never gets
> my hands on Albany again.
>
> Can anyone help?
> Thank you
> Carolyn
>
> ______________________________________________________________________________
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.

Janet Elmore on wed 9 aug 00


If you are looking for ANYTHING, try using www.google.com as your search
engine.

Below is just part of the result from typing in "oatmeal matte" to that
site.

Good luck

Janet Elmore
---------------------------------------------------

Google result follows:
Mark Issenberg on sun 21 dec 97 (ashpots@juno.com)
Les here is I used a long time ago when I fired cone 6. I used Miami
Clays # 10 it has lots of specks also Standards # 112 which I all used.
Tizzy F
Flint 463

Frit 3134 1770
Custer 300
EPK
420
Opax 295
Bent. 59

Try different tests using Red Iron Ox like 3% to 5%

On another
note , Marshall a mug is in the mail I made it at Lee Marshalls in
Tenn.It is a copper red on porcelin I hope you like itI hope this mug
doesnt put you into a higher tax bracket
also if Lee Marshall is out there, send me your E Mail adress About
the bamboo I have, It is yellow with green stripes and I also have one
called Wammin It looks like Budda Belly but stays small like 16 feet and
the nodes really swell, I have less of that, I had brought a duffle bag
of cuttings when I went to Arrowmont Clay Two the went quickly for free


Mark in Miami



SHEATEK on sun 21 dec 97 (SHEATEK@aol.com)
Here's an "oatmeal" glaze you might like, for ^6 ox. -
Sandy Tan matte:
26 custer spar
3 (%) flint
4.5 zinc oxide
7.5 kaolin
9.5 whiting

add 1.5 rutile

Happy Holidays!!
Tracy Shea