Linda Hughes on thu 27 jul 00
Hey Craig,=20
We have been playing around with a blue celadon recipe at the Kirkalnd =
Arts Centter for a while now. You know what's funny I dont' even =
remember where we got it. It does turn out to be a nice light blue on =
Seatle Pottery's Columbia White clay body. Others in the Center have =
tried it on Clay Art Center's BC10, and still others on SPS's Sculpture =
Buff. We have tried it with both G200 and Custer. See what you come up =
with.
Potash feldspar 45.40
flint 34.06
whiting 22.70
EPK 11.26
Red Iron Oxide 0.76
Have fun, Linda
| |
|