Alisa and Claus Clausen on sun 6 aug 00
This test was fired to cone 6, oxidation, on a light grey mid range =
stoneware.
Receipe =20
14 Bone ash
8 Dolomite
4 Gerstely Borate
4 Lithium Carb.
52 Custer spar
6 Kaolin=20
12 Silica
ADD
8 R.I.O.
Custer spar was substituted with my local Forshammer spar
Results were a semi glossy rather dull brown. The color is a flat dark =
brown, almost black where thickest.
Did not drip or run.
| |
|