Here's an easy ^6 white satin to glossy glaze. It does need to be =
sieved, as it contains wollastonite.
20 Ferro frit 3134
20 EPK
20 Silica
20 Custer Spar
20 Wollastonite
add: 5-15% Zircopax (I use 7%, which does show the brown clay body I =
favor. If you want opaque, I'd go with 15%.)
This recipe, created by Tony Hansen, is also available, explained in =
depth at the digital fire site. I believe the address is =
www.digitalfire.com . If that doesn't work, do a search. You'll find it =
easily. If you like it, you should probably send the cookies to him. =
He's the one who earned them.