Alisa and Claus Clausen on fri 22 sep 00
Source
Two receipes from Clayart archives, Doug Adam's Clear and Speckled Blue
Tested on light grey mid range stoneware, fired to 1220c oxidation
Receipes
Speckled Blue
50 Gerstly Borate
35 Flint
30 EPK
Add
2 Colb. oxide
Doug Adam's Clear renamed Easy Clear
48 Gerstely Borate
30 Silica
Kaolin 22
Tested receipe
Easy Clear with 2% cobalt.
Shiny, coblat blue, stable.
Best regards,
Alisa
In the archives I found several receipes that come close to Easy Clear =
in materials and amoutns, with different colorants.
To simplify thing, I mixed up the Easy Clear with the colorant procents =
of the other receipes. In the next kiln.
Best regards,
Alisa in Denmark
| |
|