Alisa and Claus Clausen on fri 22 sep 00
Source: Clayart Archives, semi gloss opaque purple
Tested on light grey mid range stoneware, fired to 1220c oxidation.
=20
Receipe=20
34 Custer spar
18 Gerstely Borate
11 Ball clay
14 Talc
10 Flint
6 Dolomite
4 Zircopax
=20
Add
3 Colb. carb.
=20
Stable, semi gloss, opaque tonedd down blue with a appealing purble/grey =
cast.
Nice.
=20
Best regards,
Alisa in Denmark
| |
|