Tested on light grey, mid range stoneware.

Gerstley Borate 46,08 %
EPK 22,55
Silica 29,41
Soda Ash 1,96

ADD=20
Red Iron Oxide 9,80

Adustments
all ingredients measured up to the next highest whole decimal.

Substitued colemanite for G.B.
Does not work.
I know it is almost 50% part of the receipe, but wanted to try it.
Glaze looks underfired, mud brown.