Alisa and Claus Clausen on fri 22 sep 00
Receipe source is Clayart Archives, Paul Lewing.
=20
Tested on light grey mid range stoneware fired to 1220c oxidation.
=20
Receipe
27 Custer spar
9 EPK
21 Whiting
18 Silica
9 Frit 3134
8 Talc
8 Gertely Borate
=20
Subs. were local frit and spar.
=20
Clear, stable, shiny gloss. No noticeable differences where double =
dipped. Some crystals where especially thick under rim.
Nice.
=20
Same receipe tested with 8 colemanite for Gerstley Borate.
No discernable difference, expect colemantite version had a very small =
bluish pool in test bowl center.
I think this sub. works.
Best regards,
Alisa in Denmark
| |
|