search  current discussion  categories  glazes - cone 4-7 

glaze test for waxy white, cone 6, reduction.

updated sat 23 sep 00

 

Alisa and Claus Clausen on fri 22 sep 00


Source Marica Selsor, Montana University, Billings

Tested on light grey, mid range stoneware, Oxidation.

Receipe

20 Gerstely Borate
30 Neph. Sye
13.3 EPK
9.4 Whiting
17.4 Talc
10 Silica
15 Zircopax

Measured up the Talc to 18.

Semi mat, white stable glaze. Good feel.
Colorant tests are in next firing.