Tested on light grey mid range stoneware, fired at 1220c oxidation.
=20
Receipe
40 Custer
9 Frit 3124
16 Whiting
9 Talc
10 EPK
16 Flint
=20
Subs are local frit and spar.
=20
Clear satin matt, Stable and did not drip. Some white crystals where =
it was double dipped.
Nice.

Same receipe with added 1% cobalt.
Shiny blue with lavender crytals.

=20
Best regards,
Alisa in Denmark
=20
=20

Sandra K Tesar on sun 24 sep 00


Thank you for a concise and clear presentation of all those glazes.
Sharing them with us all is quite a gift.
Sandy T. on Keel Mountain in North Alabama, USA
________________________________________________________________
YOU'RE PAYING TOO MUCH FOR THE INTERNET!
Juno now offers FREE Internet Access!
Try it today - there's no risk! For your FREE software, visit:
http://dl.www.juno.com/get/tagj.