search  current discussion  categories  glazes - cone 4-7 

glaze test for easy clear, cone 6 ox. with colmonite sub. for g.b.

updated sat 7 oct 00

 

Alisa and Claus Clausen on fri 6 oct 00


Source: Clayart archives, Doug Adam's Easy Clear
Tested on light grey mid range stoneware, fired to 1220c oxidation
Grogged bdy with 20% 0-1mm grogg.

Doug Adam's Clear renamed Easy Clear
48 Gerstely Borate
30 Silica
Kaolin 22


Subbed Colemanite for G.B.
Unsucessful. Resulted in a yellow/brown, dry, underfired glaze.