search  current discussion  categories  glazes - misc 

help with a lost glaze

updated wed 8 nov 00

 

Patrice Murtha on tue 7 nov 00


I'm pretty sure I got this glaze from Clayart. Can anyone help me locate a
glaze? I think it was called Pam Fredericks ^6 (It was suppose to be great
in salt)

Wade Blocker on tue 7 nov 00


Patrice,
The glaze, Pam Fredericks is in Val Cushings book. page 127

Cone 6 to cone 9

Nepheline Syenite 44.00
Gerstley Borate 12.00
Whiting l2.00
Lithium Carbonate 6.00
EPK 13.00
Flint 13.00

Add Titanium Dioxide 11.00

Hope this helps Mia in ABQ