Pancioli on wed 22 nov 00
Here is a glaze very similar to Satin Doll. It is a VERY beautiful
satin matte.
Black Satin Matte (BSM) Cone 10 Reduction
Potash Feldspar 20
Kona Feldspar 20
Whiting 2
Dolomite 15
Talc 13
Ball Clay 10
Flint 20
_______
100
Colorants Chrome 1%
Red Iron 3%
MnO2 2%
Cobalt Ox. 3%
If you want a black silvery speckle in it, use granular Manganese.
Diana
| |
|