Source: F. Carlton Ball (Mia in ABQ.)

Tested on white, mid range stoneware, fired to 1220c, oxidation.

Receipe
44 Feldspar
5 Zinc Oxide
19 Colemanite
6 Dolomite
2 Whiting
5 KY Clay
19 Flint

Substitutions
Ball clay for KY Clay

Resulted in stable, soft whitish, glossy glaze. No discernable =
difference where double dipped.