Alisa and Claus Clausen on sun 26 nov 00
Source: Cindy Strnad, USA
Tested on white, mid range stoneware, fired to 1220c, oxidation.
Receipe
20 Frit 3134
20 EPK
20 Silica
20 Custer Spar
20 Wollastonite
ADD
5 to 15% Zircopax
Substitutions
Local Frit for 3134
Local spar for Custer
used 12% Zircopax
Resulted in stable, smooth, wihte glaze.
Personal: Easy glaze and good results. Good liner or gloss white. =
Thanks Cindy!
Best regards,
Alisa in Denmark
Cindy Strnad on mon 27 nov 00
Hi, Alisa.
You're welcome. It's one of my workhorse glazes, but I can't take credit for
it. That goes to Tony Hansen. I'm glad it worked for you.
Cindy Strnad
Earthen Vessels Pottery
RR 1, Box 51
Custer, SD 57730
USA
earthenv@gwtc.net
http://www.earthenvesselssd.com
| |
|