Alisa and Claus Clausen on mon 27 nov 00
Source: Lubbock, Texas, USA
=20
42 Soda Feldspar
24 Colemanite
14 Ball clay
7 Silica
7 Ultrox
5 Dolomite
=20
ADD
5 Cobalt oxide
1.0 Chrome oxide
=20
Substitutions
Local spar for Sodaspar
Zircopax for Ultrox
=20
Resulted in dark blue to almost black, gloss. =20
=20
=20
Personal:
BUT, I do not know what this glaze ate for breakfast, but it spit all =
over like crazy. It jumped over to a pot next to the test and left a =
huge halo of blue on the
shelf and on the adjacent wall.
=20
Best regards,
Alisa in Denmark
| |
|