glaze test for rosenrot red #2 revision, cone 6 oxidation

updated tue 28 nov 00

 

Alisa and Claus Clausen on sun 26 nov 00


Source: William Edwards
Tested on mid range white stoneware, fired to 1220, oxidation
=20
Receipe
15 3134
15 Neph. Sye
37 Flint
16 Whiting
15 EPK
2 Strontium Carb.
=20
ADD
6 Tin
0.45 Chrome oxide
=20
Substitutions
Barium carb. for Strontium 1:1.33
=20
used 0,5 Chrome ox.
=20
Results:
Smooth, shiny celadon green base with a lot of red on the edges of the =
throwng rings. Some red speckling on the inside of bowl. Stable and =
slightly more red where thickest. NIce play of color between the red =
stridations on the green ground.
=20
Personal. Much better results then version no. 1. This glaze is a =
psuedo reduced celadon. Exciting effect for oxidation.
Will try it on porcelain next time.