Source: Willam Edwards

Tested on white, mid range stoneware, fired to 1220c, oxidation.

Receipe:

31 Frit 3134
9 Soda Feldspar
18 Talc
16 EPK Kaolin
26 Silica
2 Strontium Carb.

Substitutions:

Local frit for 3134
Local spar for sodaspar
Barium Carb. 2.66 for 2 Strontium Carb.

Resulted in stable, clear gloss.

Best regards,