Source Emanuel Cooper (Ababy Sharon)
Tested on white, mid range stoneware, fired to 1220c, oxidation.

Receipe

19.4 Barium Carb.
9.7 Whiting
9.7 Zinc. Oxide
48.6 Sodaspar
9.7 Ball clay
2.8 Rutile

Substitutions
Local spar for sodaspar

Resulted in very, very dry matt pale yellow that clung very closely to =
the test bowl, like a slip,
Looks like an underfired surface, but very smooth. Could be interesting =
toghether with other detail glazes.

Best regards,