Alisa and Claus Clausen on sat 9 dec 00


SEA MIST GREEN, ^6 ox.
=20
Source Lubbock, Texas
=20
Tested on white, mid range stoneware, fired to 1220c, oxidation.
Receipe
48 Soda Feldspar
14 Ball Clay
7 Silica
7 Ultrox
5 Dolomite
6 Tin ox.
=20
ADD
2 Copper Carb.
=20
Subs. used
Local spar for Sodaspar
Zircopax for Ultrox
Titanium diox. for Tin ox.
=20
Stable, glossy, pale green glaze. Needs to be applied with a good coat, =
otherwise buttery yellow where thin.
Personal: Appealing light green with some fluctutions in intensity =
througout glaze.