Mountain Rock, C6, oxidation.
Tested on mid range, iron flecked Stoneware, fired to 1220c, oxidation.

Receipe for base glaze Matt.

230 G200
30 EPK
20 Whiting
20 Frit 3134

ADD
12 RIO

Resulted in a veriegated brown, with many nuances of rust brown and =
darker. VERY fluid. In fact,=20
NICE shelf on that test bowl! Ran off the test bowl. Good color, very =
unstable. Could use maybe inside
a large bowl.

Best regards,
Alisa in Denmark