search  current discussion  categories  glazes - cone 4-7 

glaze test for zakins satin whjite, c6, oxidation.

updated fri 22 dec 00

 

Alisa and Claus Clausen on thu 21 dec 00


Tested on mid range, iron felcked stoneware, fired to 1220c, oxidiation.
=20
Receipe
18 Custerspar
20 Soda Frit
14 Spodumene
10 Kaolin
14 Dolomite
24 Zirocopax
=20
Subbed local spar for Custer
Subbed loca frit for Soda frit
=20
Resulted in a semi matt, covering white, stable glaze.
=20
Best regards,
Alisa in Denmark