Pancioli on tue 27 feb 01
Patrice:
Are you looking for a reduction celadon or an oxidation "celadon" at
cone 6?
Diana
Ron Collins on thu 28 mar 02
As another addition to old worn out threads, here is the best cone 5 or =
6 celadon I have ever used, taken from clayart archives, it's frosty, =
not glossy, and takes other colorants well, in small amounts. Also, =
inexpensive to make...can settle, so I add epsom salts.....just a lovely =
glaze...
Birke's Celadon-cone 5-6 oxidation-fake celadon, really
Feldspar--58 doesn't say what kind, again having to use my =
unspecified
Whiting-17
Flint-14
Ball clay-6
Zinc oxide-5
Copper carb-1/2 percent
Melinda
Lynne Berman on mon 12 jul 10
Just recovered from a week with John Britt. He worked us hard and we
are drowning in test tiles. We had a wonderful and productive time.
The studio (Long Beach Island Foundation of the Arts and Sciences)
celadon looked great at ^6 as did most of our ^10 glazes. Yours may too.
Here it is:
CAC Celadon
Custer Feldspar 442
Whiting 54
EPK 35
Flint 223
Strontium 120
Plus:
Red Iron Oxide 10
Bentonite 20
Lynne Berman
Johanna San Inocencio on tue 13 jul 10
--=3D=3D=3D=3D=3D=3D=3DAVGMAIL-37F704FA=3D=3D=3D=3D=3D=3D=3D
This is a multi-part message in MIME format.
Content-Type: text/plain; charset=3DISO-8859-1; format=3Dflowed
Content-Transfer-Encoding: 7bit
Do you have any pictures of the test tiles? I would love to see them.
Johanna
"A man is as free as he chooses to make himself,
never an atom freer."
The Raven, Lillith by George MacDonald
On 7/12/2010 4:32 PM, Lynne Berman wrote:
> Just recovered from a week with John Britt. He worked us hard and we
> are drowning in test tiles. We had a wonderful and productive time.
>
> The studio (Long Beach Island Foundation of the Arts and Sciences)
> celadon looked great at ^6 as did most of our ^10 glazes. Yours may too.
> Here it is:
>
> CAC Celadon
>
> Custer Feldspar 442
> Whiting 54
> EPK 35
> Flint 223
> Strontium 120
>
> Plus:
> Red Iron Oxide 10
> Bentonite 20
>
> Lynne Berman
>
>
>
> No virus found in this incoming message.
> Checked by AVG - www.avg.com
> Version: 9.0.830 / Virus Database: 271.1.1/3001 - Release Date: 07/12/10 =
11:49:00
>
>
--=3D=3D=3D=3D=3D=3D=3DAVGMAIL-37F704FA=3D=3D=3D=3D=3D=3D=3D
Content-Type: text/plain; x-avg=3Dcert; charset=3Dus-ascii
Content-Transfer-Encoding: quoted-printable
Content-Disposition: inline
Content-Description: "Certification"
No virus found in this outgoing message.
Checked by AVG - www.avg.com
Version: 9.0.830 / Virus Database: 271.1.1/3001 - Release Date: 07/12/10 11=
:=3D
49:00
--=3D=3D=3D=3D=3D=3D=3DAVGMAIL-37F704FA=3D=3D=3D=3D=3D=3D=3D--
| |
|