Ababi on sun 4 mar 01
Clay Times1/2/99
Great glaze recipes
Copper Bronze Raku ^04
G.B. .................50
Frit 3134..........50
Add tin..............5.1
Copper Oxide...4.3
Reduce in newspaper well closed until cool
In an article by Charlie Riggs and J.D. Riggs in the same issue I post here
the ^04 recipe
G.B.
Charlie Crackle raku ^06-^04
G.B...............42
Potash feldspar...........32.5
Frit 3289......................15
Silica............................10.5
For blue:0.5Cobalt c.
Emerald green 3-6 copper C.
Please pass it to Charlie Riggs.
One has to fight to develop himself.
and know his limits.
Perhaps I can do some of the great works\glazes of Charlie teaches in the
magazines. For sure I enjoy very much looking at them through Clay Times and
the net.
Ababi Sharon
ababisha@shoval.ardom.co.il
http://members4.clubphoto.com/ababi306910/
----- Original Message -----
From: "Diane Echlin"
To:
Sent: Saturday, March 03, 2001 1:47 AM
Subject: Re: Searching for Witt ^04 Electric Raku Glaze Recipe
> sorry, can't help, but try the clayart archives. The url is on the bottom
of all
> the clayart mail.
> Good luck!
>
> "K.Wilson" wrote:
>
> > I have been trying to get a copy of this glaze recipe - I know it
> >
> > was in ClayTimes Jan/Feb 99 issue, but I don't have copies that
> > far back. I have tried the libraries, but they don't even carry
> > the magazine! Does anyone have it?
> >
> > Thanks,
> > Katherine
> >
> >
____________________________________________________________________________
__
> > Send postings to clayart@lsv.ceramics.org
> >
> > You may look at the archives for the list or change your subscription
> > settings from http://www.ceramics.org/clayart/
> >
> > Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>
>
____________________________________________________________________________
__
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at
melpots@pclink.com.
>
| |
|