Tested on light, iron flecked, mid-range stoneware, fired to 1215c, soak =
30 minutes, oxidation.

Receipe
40 3134
30 Kaolin
20 Wollastonite
10 OM4 Ball
8 Tin Oxide

Subs:
Frit 169 for 3134
Nr.3, TWVD Ball for OM4

Resulted in a stable, white, semi gloss glaze. the edges are very =
organey and toasty. The iron flecks showed through the glaze with a lot =
of nice streaking and falling. Cobalt wash also showed through with =
indefinte boarders.
William fires to a flat six with a digital kiln and that the materials =
he uses are exacting for what he analyzes them to be in his receipes.

Best regards,
Alisa in Denmark