William Edwards Matt with Dolomite=A9 , cone 6, oxidation.
Tested on light, iron flecked, mid-range stoneware, fired to 1215c, soak =
30 minutes, oxidation.
40 Frit 3124
30 EPK Kaolin=20
20 Dolomite
10 Flint
Resulted in a stable semi gloss with a slightly greenish tinge =
throughout. Covering, although the iron flecks were visible and =
slightly streaking.
Kiln was fired hot, so it may be more of matt in a true cone 6 firing.
William fires to a flat six with a digital kiln and that the materials =
he uses are exacting for what he analyzes them to be in his reecipes.