search  current discussion  categories  glazes - specific colors 

=?iso-8859-1?q?glaze_test_for_williiam__edwards_white_bear=a9=2c_cone_6?=

updated fri 16 mar 01

 

Alisa og Claus Clausen on thu 15 mar 01

=?iso-8859-1?Q?=2C_oxidation.?=

Edward Williams White Bear=A9 , cone 6, oxidation.

Tested on light, iron flecked, mid-range stoneware, fired to 1215c, soak =
30 minutes, oxidation.

Receipe
40 3124
30 Kaolin
20 Wollastonite
10 Flint
8 Tin Oxide

Subs.
Frit 169 for 3124

Since William noted that Frit 3124 is crucial to this glaze, my sub. =
with 169 produced a glaze that was a stable, clear gloss, probably not =
much like the original glaze. =20
=20
William fires to a flat six with a digital kiln and that the materials =
he uses are exacting for what he analyzes them to be in his reecipes.
..

Best regards,