glaze test for pink matt, cone 6, oxidation

updated fri 16 mar 01

 

Alisa og Claus Clausen on thu 15 mar 01


Matt Pink, cone 6
Source Clayart

Tested on light, iron flecked, mid-range stoneware, fired to 1215c, soak =
30 minutes, oxidation.

Receipe
15.2 Barium Carbonate
10.2 Gerstely Borate
15.2 Wollastonite
38.7 Neph. Syenite
10.2 EPK
10.5 Flint

ADD
10% pink stain

All precents measured up or down to nearest whole decimal.

Resulted in a pink matt. Stable, covering and slightly dry where =
thickest. Absolute freshly hosed off piglet color.

Best regards,
Alisa in Denmark