Alisa og Claus Clausen on thu 15 mar 01
Tony's Ulta Clear, cone 6, oxidation. =20
Source: Tony Martens, South Africa
Tested on light, iron flecked, mid-range stoneware, fired to 1215c, soak =
30 minutes, oxidation.
Receipe
25 EPK Kaolin
20 Feldspar
30 3134
15 Silica
10 Wollastonite
Feldspar used is Forshammer.
Resulted in an absolute clear gloss, stable. Iron flecks showed through =
slightly streaking.
Best regards,
Alisa
| |
|