search  current discussion  categories  events - nceca 

cone ^6 shino ; was: re: back from nceca... wow!

updated fri 6 apr 01

 

Lee Love on thu 5 apr 01


----- Original Message -----
From: "L. P. Skeen"

> one on my bowl I think was a reduction glaze. Have you tried any ^6R
> shinos? I don't think I hve ever heard of any recipes for that, but
> wondered.

Here are a couple Shinos we woodfired with In New London. The first is a cone 6, can be used in the cooler places of the kiln,
but can take a higher temp. It can be mixed with the cone 10 glaze, different mixes for the temperature of the kiln area.

Shino Translucent Glaze ^6 Redu Craig Edwards

Gerstley Borate 5
Soda Ash 4
Spodumene 22
Neph Sye 54
OM4 15
Bentonite 1.5

Good over Iron Wash

^10 Shino

Soda Ash 10
Spodumene 40
Neph Sy 40
OM4 10
Benonite 1.5

--

Lee Love
Mashiko JAPAN Ikiru@kami.com
Interested in Folkcraft? Signup:
Subscribe: mingei-subscribe@egroups.com
Or: http://www.egroups.com/group/mingei
Help ET phone Earth: http://setiathome.ssl.berkeley.edu/