glaze, cone 6, oxy, floating green

updated mon 9 apr 01

 

Cindy Strnad on sun 8 apr 01


Floating Green ^6

===================
NEPHELINE SYENITE... 30.00 29.13%
GERSTLEY BORATE..... 21.00 20.39%
WHITING............. 8.00 7.77%
EPK KAOLIN.......... 10.00 9.71%
FLINT............... 31.00 30.10%
*Chrome Oxide........ 2.00 1.94%
*Cobalt Oxide........ 1.00 0.97%
========
103.00

CaO 0.63* 11.59%
MgO 0.07* 0.89%
K2O 0.05* 1.68%
Na2O 0.24* 4.95%
TiO2 0.00 0.04%
Al2O3 0.38 12.63%
B2O3 0.31 6.95%
P2O5 0.00 0.03%
SiO2 3.11 61.05%
Fe2O3 0.00 0.18%

Cost/kg 1.06
Si:Al 8.21
SiB:Al 9.01
Expan 7.39


I tested this one (found at www.frogpondpottery.com ) for my own benefit,
but am including it for general interest. I know most of us are gerstley
free these days. In case you have a nice stash, however, this is a gorgeous
glaze. It turned out a rich, soft gloss emerald green with floating gray
flecks. Worth the use of my precious GB, or of experimentation with
substitutes, in my opinion.