glaze test edward's 1.2.3.4 clear gloss

updated sun 10 jun 01

 

Marianne Lombardo on fri 8 jun 01


So far, this is the nicest clear gloss glaze I've tried. I've used it =
three times now, and each time I am very happy. My underglaze colors =
come out so clean and no distortion. Two light coats of this glaze =
works well for me. (Applied with brush. I brush all my glazes, =
actually). No pinholes, doesn't run, doesn't seem to be especially =
picky about slow or fast cooldowns.

William Edward's 1.2.3.4 Clear Gloss
30.0 EPK
20.0 Flint
40.0 Frit 3134
10.0 Wollastonite

I have not tried any colorants with this glaze yet. But as a clear =
glaze to apply over underglaze brushwork, I don't need to look any =
further or test any more. This is a keeper. Now I have to try some =
matte glazes over my underglaze brushwork and see if I can find a nice =
clear, matte. =20

Marianne Lombardo
Omemee, Ontario, Canada
email: mlombardo@nexicom.net