Marty Morgan on wed 8 aug 01
Awhile ago I tested a receipe for "Tom Coleman's no-craze white". It looked
great on Miller's #900 cone ten clay. I think it was in Ceramics Monthly,
but can no longer find it. Anyone out there know the receipe?
Marty
Gloucester, MA
GORMO1@AOL.COM on wed 8 aug 01
^10-11 (R) no craze white (tom coleman)
custer 29.90
whiting 11.34
talc 11.34
epk 26.80
flint 20.63
Si: Al 6.58
Sib:al 6.58
expan 6.09
here you go
jim gorman
| |
|