.Woo yellow from Penland school.
WOO YELLOW 1201deg.C. Cone 6
------------------------------------------------------------------------
----------------------------
Formula Weight% Recipe
------------------------------------------------------------------------
----------------------------
KNO 0.1979 4.32% FELDSPAR SODA F7/SE 36.00
CaO 0.2643 5.16% Barium Carbonate 20.00
MgO 0.2065 2.90% Dolomite 13.00
BaO 0.3313 17.68% EPK Kaolin 8.00
Al2O3 0.2987 10.59% SILICA 8.00
P2O5 0.0004 0.02% ULTROX 15.00
SiO2 2.2882 47.84% Red Iron Oxide 3.00
ZrO2 0.2676 11.47%
TiO2 0.0012 0.03%
K2O 0.0044 0.14%
Na2O 0.1935 4.17%
Al:Si 7.6605
Expan. 8.4461
ST 372.383
-----
Beautiful pal matte yelow. Use it above mottled claybody the
dots are seen thrugh.
BUT!!!
WOO YELLOW2 1201deg.C. Cone 6
------------------------------------------------------------------------
----------------------------
Formula Weight% Recipe
------------------------------------------------------------------------
----------------------------
KNO 0.1977 4.58% FELDSPAR SODA F7/SE 36.00
CaO 0.2640 5.47% STRONTIUM CARBONATE 15.00
MgO 0.2063 3.07% Dolomite 13.00
SrO 0.3319 12.70% EPK Kaolin 8.00
Al2O3 0.2984 11.23% SILICA 8.00
P2O5 0.0004 0.02% ULTROX 15.00
SiO2 2.2860 50.73% Red Iron Oxide 3.00
ZrO2 0.2673 12.16%
TiO2 0.0012 0.04%
K2O 0.0044 0.15%
Na2O 0.1933 4.43%
Al:Si 7.6605
Expan. 8.5563
ST 387.058
Here without the barium. Looks and feels the same without the Barium.
Ababi Sharon
Kibbutz Shoval- Israel
Glaze addict
ababisha@shoval.org.il
http://members4.clubphoto.com/ababi306910/
http://www.milkywayceramics.com/cgallery/asharon.htm
http://www.israelceramics.org/
| |
|