search  current discussion  categories  materials - barium 

pete's strontium green matt

updated thu 29 nov 01

 

Lesley Alexander on wed 28 nov 01


Hi John et al, Maybe Pete's Weathered Bronze Green isn't the same as
his strontium matt, which is listed below. Can someone post it? I've
been skipping those emails because I thought it was a ^6 glaze only. The
archives doesn't have it listed per se. Lesley

** Pete’s Strontium Matt
Neph Sy 20
Lithium 1
Ball Clay 10
Stront carb 20
Silica 9
Bentonite 2%
For Green add cu carb 5%, Tit dioxide 5%
For Grey ad tit diox 5%
For Turquoise add Cu carb 5%