I have a recipe from Marcia Selsor I tested a long time ago.
It is cone 6, reduction. I tested it in oxidation, with results in archives.
It should be tomato iron red with gold flecks in the sun when fired in redux.
In oxidation it was brown, just brown.


14 Bone Ash
8 Dolomite
4 G.B.
4 Lithium Carb.
52 Custer spar
'6 Kaolin
12 Silica

ADD
8 RIO

best regards,
Alisa in Denmark

Marcia Selsor on thu 6 dec 01


I submitted that to Mike Bailey's new book on ^6 reduction gllazes. It IS a tomato
red in reduction. I never tried it in OX.
Marcia Selsor

Alisa og Claus Clausen wrote:

> I have a recipe from Marcia Selsor I tested a long time ago.
> It is cone 6, reduction. I tested it in oxidation, with results in archives.
> It should be tomato iron red with gold flecks in the sun when fired in redux.
> In oxidation it was brown, just brown.
>
> 14 Bone Ash
> 8 Dolomite
> 4 G.B.
> 4 Lithium Carb.
> 52 Custer spar
> '6 Kaolin
> 12 Silica
>
> ADD
> 8 RIO
>
> best regards,
> Alisa in Denmark
>
> ______________________________________________________________________________
> Send postings to clayart@lsv.ceramics.org
>
> You may look at the archives for the list or change your subscription
> settings from http://www.ceramics.org/clayart/
>
> Moderator of the list is Mel Jacobson who may be reached at melpots@pclink.com.