i add here both recipes the original and the one i converted to red

updated sat 26 jan 02

 

Ababi on fri 25 jan 02

art.

I add here both recipes the original and the one I converted to red art.
Falls creek Zinc (ababi -11)
============================
RED CLAY............ 43.4 43.44%
ULTROX.............. 8.2 8.20%
TIN................. 4.1 4.10%
FRIT 3134........... 27.0 27.05%
WHITING............. 2.5 2.46%
ZINC OXIDE.......... 8.2 8.20%
QUARTZ.............. 6.6 6.56%
========
100.0

CaO 0.40* 7.32%
MgO 0.04* 0.55%
K2O 0.08* 2.39%
Na2O 0.15* 3.04%
ZnO 0.33* 8.67%
TiO2 0.02 0.48%
ZrO2 0.14 5.63%
Al2O3 0.28 9.42%
B2O3 0.29 6.61%
SiO2 2.70 52.67%
Fe2O3 0.06 3.21%

Text1 13.82
Si:Al 9.49
SiB:Al 10.52
Expan 7.11

Notes:


TO TEST WITH DIFFERENT OXIDES ON BUFF CLAYBODY

Here with redart:
Falls creek Zinc (ababi -11)
============================
ULTROX.............. 7.9 7.93%
TIN................. 4.0 3.97%
FRIT 3134........... 26.2 26.17%
WHITING............. 2.4 2.38%
ZINC OXIDE.......... 8.0 8.03%
QUARTZ.............. 4.1 4.12%
REDART.............. 38.7 38.70%
CUSTER FELDSPAR..... 2.9 2.90%
EPK KAOLIN.......... 5.8 5.81%
========
100.0

CaO 0.40* 7.27%
MgO 0.05* 0.67%
K2O 0.07* 2.09%
Na2O 0.16* 3.18%
ZnO 0.33* 8.69%
TiO2 0.02 0.48%
ZrO2 0.14 5.58%
Al2O3 0.28 9.42%
B2O3 0.29 6.55%
P2O5 0.00 0.11%
SiO2 2.70 52.95%
Fe2O3 0.06 3.01%

Text1 12.50
Si:Al 9.54
SiB:Al 10.56
Expan 7.04

Notes:


TEST WITH DIFFERENT OXIDES ON BUFF CLAYBODY
As I wrote before, on Sunday I will be smarter
Good luck
Ababi