search  current discussion  categories  glazes - cone 4-7 

glaze test for oribe, cone 6, ox.

updated mon 11 feb 02

 

Alisa og Claus Clausen on sun 10 feb 02


Glaze test for: Oribe, cone 6, ox.

Source: www.frogpondpottery.com
Credited to:

All tests fired on white, iron flecked, mid-range stoneware.
Fired to cone 6 (1220c) in oxidation.

Firing ramp:
100c (212f) per hour to 600c (1112f)
150c (302f) per hour to 1100c (2012f)
100c per hour to 1220c (2228f)
15 - 30 minute soak depending on matts and glosses used.
cool down 100c per hour to 900c.
Natural cool down to 150c (approximately 15 hours)

Recipe:
28 Custer Feldspar
19Whiting
7 Frit 3195
13 Ball Clay
33 Flint

ADD
4.5 Copper Carb.

Note:
All raw materials measured up or down to nearest whole decimal.
Oxides used on percent basis to a 100 gram batch of glaze.

Substitutions:
Forshammer Feldspar for Custer
Local Frit for 3195

Resulted in:
A semi matt glaze that is well covering and stayed where glazed. A fine
copper green color, with a smooth surface.
A glaze I would like to test on larger ware.

Regards from Alisa in Denmark