Alisa og Claus Clausen on sun 10 feb 02
Glaze test for: Teal Blue, cone 6, ox.
Source: www.frogpondpotter.com
Credited to: Jane Deboos
All tests fired on white, iron flecked, mid-range stoneware.
Fired to cone 6 (1220c) in oxidation.
Firing ramp:
100c (212f) per hour to 600c (1112f)
150c (302f) per hour to 1100c (2012f)
100c per hour to 1220c (2228f)
15 - 30 minute soak depending on matts and glosses used.
cool down 100c per hour to 900c.
Natural cool down to 150c (approximately 15 hours)
Recipe:
35 Nepheline Syenite
30 Silica
18 Whiting
12 Frit 3134
5 Ball Clay, OM4
ADD
8 Tin Oxide
4 Copper Carbonate
Note:
All raw materials measured up or down to nearest whole decimal.
Oxides used on percent basis to a 100 gram batch of glaze.
Substitutions:
Ball Clay not OM4.
Resulted in:
A well covering gray toned teal blue gloss.
Regards from Alisa in Denmark
| |
|