search  current discussion  categories  glazes - specific colors 

berry rust addendum

updated tue 26 feb 02

 

Carol Tripp on mon 25 feb 02


I forgot to mention the following in connection with my use of Berry Rust;

Clay: Tuckers Smooth White and/or Mid Red ^6
Glaze seived once through 80 mesh
Fired to self supporting Orton Cone 6 tip touching shelf
Soak - this varies with kiln behaviour, I shut the soak off when the cone
falls
I fire down using a controller as my 2 1/2" kiln drops like a rock; 50C an
hour until 700C then 30 min soak and then off
Passes home vinegar test