Forest Green ^6
(see notes in separate post on firing specifics)
Frit 3134 50
Silica 25
EPK 25
Chromium Oxide 1
Cobalt Oxide 0.5
Very nice glossy forest green. Needs to be fairly thick for good color on my
brown clay, but if you get it too thick, it will run.
=====================================