search  current discussion  categories  glazes - faults 

tony hanson 5x 20 glaze crawling

updated wed 3 apr 02

 

Leslie St. Clair on tue 2 apr 02


I was also having some crawling problems with this
glaze, and so I tested and starting using the Ron Roy
revision.
Here it is:
G200 or Custer feldspar 18
wollastonite 19.5
frit 3134 19.5
om#4 ball clay 28
silica 15

I haven't tried it with zircopax, but this glaze
flows more smoothly, isn't dusty when dry, doesn't
pinhole or crawl, and in general handles better than
the 5x20 glaze. I would definately try this one to
solve your crawling problem.
Good luck,
Leslie St. Clair in Ft. Mitchell, KY