search  current discussion  categories  glazes - traditional iron glazes 

john baymore's shino

updated mon 15 apr 02

 

Lee Love on sun 14 apr 02


John Baymore's Spod and Neph Syn-less Shino: Japanese materials I
substituted
directly:

261-F Spar 68.7 Kamado Feldspar
OM4 Ball Clay 17.2 Gariome Ball Clay
EPK 9.8 (Korean)Kanpaku Kaolin
Soda Ash 4.3 Soda Ash

From ultimate source:

CaO .1028
MgO .00344
K2O .06297
Na2O .0448
AL2O3 .11314
SiO2 1.1568
Fe2O3 .00036

Japanese materials analysis:

Kamado Gairome Korean Kaolin

SiO2 74.42 69.20 45.82

Al203 13.62 17.83 37.27

Fe2O3 0.14 `1.73 0.53

CaO .072 0.11 0.60

MgO 0.06 0.78 0.25

K2O 5.24 2.03 0.54

Na20 4.77 0.99 0.46

Ig Loss 0.83 6.19 14.42