favorite glaze forgot the cone silky matt

updated wed 8 may 02

 

chris clarke on tue 7 may 02


Sorry everyone, I was in such a rush I forgot to list the cone and
atmosphere, so here is my original post plus the temp. I got several emails
but none were mean, thanks.

Silky Matt from the digital fire book.

Takes colors wonderfully and is a lovely white. When I first tried it out I
sat with the test piece in my hand for a hour because it is so smooth. Four
ingredients.

Silky Matt **CONE 10 REDUCTION**

custer feldspar 33
dolomite 23
kaolin 22
silica 22

I love it.

chris



temecula, california
chris@ccpots.com