search  current discussion  categories  glazes - traditional iron glazes 

chun white - correction

updated wed 15 may 02

 

Lesley Alexander on tue 14 may 02


Kristin kindly pointed out I'd entered EPK twice in my chun white
recipe. The higher epk number was supposed to be Gerstley Borate.
Ooops. The un-guru strikes again.

Here is the recipe again, adding up to 100, plus zircopax. I can't say
if it's the best choice... just that I like it.

"Strontium Chun White"
CUSTER FELDSPAR..... 46.97 43.69%
EPK KAOLIN.......... 1.44 1.34%
WHITING............. 2.60 2.42%
DOLOMITE............ 8.76 8.15%
Gerstley Borate..... 8.76 8.15%
STRONTIUM CARBONATE. 3.37 3.13%
zinc................ 1.73 1.61%
SILICA.............. 26.37 24.53%
ZIRCOPAX............ 7.50 6.98%
========
107.50